시동/정지 반복에 따른 고분자전해질 연료전지의 성능 저하에 관한 연구
- Other Titles
- A Study on Performance Degradation of PEMFC by Repetitive Startup/Shutdown Cycling
- Authors
- 조유연; 조은애; 김정현
- Issue Date
- 2009-08
- Publisher
- 한국수소및신에너지학회
- Citation
- 한국수소및신에너지학회논문집, v.20, no.4, pp.317 - 322
- Abstract
- To investigate degradation mechanism of PEMFC operated with repetitive startup/shutdown cycling,
i-V characteristics, impedance, cyclic voltamograms were measured. OCV decreased from 0.967 to 0.951 V
while the cell voltage at 800mA/cm2 from 0.657 to 0.563V, implying that the electrodes rather than
membrane electrolyte was damaged during the cycling operation. Electrochemical analyses supported that
the performance degradation could be mainly attributed to degradation of the electrodes such as a decrease
in electrochemical active surface area rather than degradation of membrane.
- Keywords
- PEMFC; Degradation; Startup/Shutdown; Dummy load; 고분자전해질 연료전지; 열화; 시동/정지; 더미 저항
- ISSN
- 1738-7264
- URI
- https://pubs.kist.re.kr/handle/201004/132255
- Appears in Collections:
- KIST Article > 2009
- Files in This Item:
There are no files associated with this item.
- Export
- RIS (EndNote)
- XLS (Excel)
- XML
Items in DSpace are protected by copyright, with all rights reserved, unless otherwise indicated.